一、开槽参数 (tank set up parameters)
DBR-603: 15~25g/L
二、控制参数 (coolling parameters)
DBR-603:15~20 g/L
温 度 (Temperature):40~50℃
PH值 (Value) : 4.8~5.1
时间 (Time ) : 1~15min
三、维护和管理 (maintenance and cool)
1.每天检测槽液中DBR-603浓度并根据分析结果及时补加调整;处理100m2约消耗DBR-603:0.6~1Kg。
Detection of the bath conceation of DBR-603, according to the analysis results to adjust and add; the DBR-603of consumption is 0.6~1Kg for each 100m2 treatment.
2.正常生产时PH值呈上升趋势,每天需检测一次PH值,并用草酸调整至工艺范围内;如PH值偏低则说明带入酸水过多,需控制染色前水洗PH值≥4.5。
The PH value rising when produce, it should measured PH value and used oxalic acid adjusted the scope of technology parameter; the acidic water is brought too much if the PH value indicated in low , it need to cool the rinse water PH value ≥ 4.5 before dying.
3.不生产时须加盖槽液以防污染;并把PH值下调至4.5且每班检测一次PH值,以防PH值过高(≥5.5)导致有效成分分解。
Covered the bath to prevent contamination when stop produce, and reduced the PH value to 4.5 not higher than PH value (≥ 5.5), lead to decomposition of active ingredients.
4.长期生产槽液或多或少会有沉淀物产生,要定期过滤或倒槽清理沉淀物。
Producing bath will produced more or less white precipitate for a long time, you need to filter or reverse the bath to clean sediments regularly.